发明名称 |
Verfahren und Vorrichtung zum Entzundern von Eisenknueppeln |
摘要 |
A process of descaling ferrous billets comprises heating the billets to an intermediate temperature e.g. 1900 DEG F., coating the billets with a dry flux, heating to working temperature e.g. 2300 DEG F. and descaling with e.g. high pressure water jets. The flux used may be a mixture of 33-67% of a glass and 67-33% of NaCl, KCl or BaCl2. The heated billets are rolled over a bed of powdered flux and then heated to 2300 DEG F. in an induction furnace in 5-15 minutes. Instead of water sprays descaling may also be carried out with rotating wire brushes. <PICT:1061806/C6-C7/1> |
申请公布号 |
DE1546084(A1) |
申请公布日期 |
1970.11.05 |
申请号 |
DE19641546084 |
申请日期 |
1964.11.23 |
申请人 |
THE BABCOCK & WILCOX CO. |
发明人 |
A. EDGECOMBE,DAVID;C. GIOFFRE,VINCENT;C. GIOFFRE,VINCENT |
分类号 |
C23G5/00 |
主分类号 |
C23G5/00 |
代理机构 |
|
代理人 |
|
主权项 |
|
地址 |
|