摘要 |
The low-reflexibility colored glass is produced by preparing one solution of 1000 cc pure water, 6 g silver nitrate, 11 cc liquid ammonia, 6 g caustic postash, 0.03 g potash dechromate and 0.01 g gold cyanide, preparing another solution of 1000 cc pure water, 4 g glucose, 0.6 cc formalin, 0.2 g potash acetate, 0.6 g soda sulfate and 0.01 g potash dechromate, spraying the two solutions on the pretreated transparent glass simultaneously to make thin film, and heat-treating at a high temparature to make a light yellow and transparent silver nitrate oxide film.
|